Polymer physics

Related Topics:

Back to Index

Refractive Index of Amorphous Polymers

Amorphous Polymer  nD1
Poly(tetrafluoroethylene), PTFE 1.356
Poly(2,2,2-trifluoroethyl acrylate) 1.409
Poly(2,2,2-trifluoroethyl methacrylate) 1.418
Poly(2,2,3,3-tetrafluoropropyl methacrylate) 1.420
Poly(vinylidene fluoride), PVDF 1.426
Poly(isobutyl vinyl ether) 1.451
Poly(oxymethylene) 1.453
Poly(ethylene glycol) 1.458
Poly(methyl vinyl ether)  1.458
Poly(pentyl vinyl ether) 1.459
Poly(vinyl methyl ketone) 1.459
Poly(hexyl vinyl ether) 1.459
Poly(octyl vinyl ether) 1.461
Poly(3-ethoxypropyl acrylate) 1.462
Poly(4-methyl-1-pentene) 1.462
Poly(isopropyl methacrylate)  1.463
Poly(ethyl vinyl ether) 1.463
Poly(tert-butyl methacrylate) 1.464
Poly(dodecyl methacrylate) 1.465
Poly(butyl acrylate), PBA 1.465
Polylactic acid, PLA 1.465
Poly(ethyl acrylate), PEA 1.467
Poly(2-ethoxyethyl acrylate) 1.474
Poly(methyl acrylate), PMA 1.476
Poly(ethylene) 1.476
Poly(vinyl formate) 1.476
Poly(isobutyl methacrylate) 1.480
Poly(hexyl methacrylate) 1.481
Poly(3-methoxypropyl acrylate) 1.483
Poly(butyl methacrylate) 1.483
Poly(propyl methacrylate) 1.484
Poly(vinyl acetate) 1.484
Poly(vinyl butyral) 1.485
Poly(methyl methacrylate) 1.491
Poly(2-ethoxyethyl methacrylate) 1.495
Poly(1-butene) 1.497
Poly(ethyl methacrylate) 1.498
Poly(2-chloroethyl methacrylate) 1.503
Poly(cyclohexyl methacrylate) 1.507
Poly(isobutene) 1.507
Poly(2-hydroxyethyl methacrylate) 1.507
Poly(tetrahydrofurfuryl methacrylate) 1.508
Poly(acrylic acid), PAA 1.508
Poly(acrylonitrile) 1.513
Poly(methyl isopropenyl ketone) 1.520
Polyisoprene 1.521
Poly(ω-dodecanamide), Nylon 12 1.525
Poly(vinyl alcohol) 1.526
Poly(N-methyl-methacrylamide) 1.529
Poly(N-methyl-methacrylamide) 1.529
Poly(caprolactam), ylon 6 1.530
Poly(hexamethylene adipamide), Nylon 6,6 1.530
Poly(vinyl chloride), PVC 1.531
Poly(2-bromoethyl methacrylate) 1.535
Poly(hexamethylene sebacamide), Nylon 6,10 1.539
Poly(1,4-butadiene) 1.539
Poly(2-phenylethyl methacrylate) 1.547
Poly(vinyl benzoate) 1.561
Poly(phenyl methacrylate) 1.561
Polychloroprene (Neoprene) 1.561
Poly(ethylene terephthalate), PET 1.575
Poly(4-methylstyrene) 1.578
Poly(2,6-dimethyl-p-phenylene oxide), PPO 1.579
Poly(Bisphenol B carbonate) 1.583
Poly(2-methoxystyrene) 1.585
Poly(Bisphenol A carbonate), PC 1.586
Poly(2-methylstyrene) 1.587
Poly(benzyl methacrylate) 1.589
Poly(methacrylonitrile) 1.590
Polystyrene, PS 1.593
Poly(2,5-dimethyl-1,4-phenylene ethylene) 1.595
Poly(propylene sulfide) 1.596
Poly(4-bromophenyl methacrylate) 1.596
Poly(N-benzyl methacrylamide) 1.597
Poly(2-chlorostyrene) 1.597
Poly(2,6,3',5'-tetrachloro bisphenol A carbonate) 1.598
Poly(vinylidene chloride), PVDC 1.615
Poly(2,6-dichlorostyrene) 1.625
Polysulfone, PSU 1.642
Poly(p-xylene) 1.669
1 The refractive indices are the average of one or more experimental values.

Refractive Index

Alphabetical